Kochlin SPECIAL ALLOYS · SINCE 2009
HomeGradesN10665

NiMo28 · UNS N106652.4617 · Alloy B-2 / Hastelloy B-2

Ni-Mo type — dedicated to hydrochloric and reducing acids

HastelloyNi corrosion-resistant
Units
Tensile Rm
760
MPa · ≥ std. min
Yield Rp0.2
350
MPa · ≥ std. min
Elongation A
40
% · ≥ std. min
Service limit
540
°C · indicative max
Density
9.22
g/cm³

Physical properties

Density9.22g/cm³

Informative values: they vary with composition, condition and test method. Use the governing standard or measured mill data for pressure and heat-transfer calculations.

Chemical composition

Ni 67%Mo 28%Minor & residual 5.2%

Nominal: mid-range where both limits are given, the cap where only a maximum is, balance takes the remainder. Exact specified ranges below.

ElementName Content %
Main elements2 elements
Ni NickelBal.
Mo Molybdenum26 – 30%
ElementName Content %
Minor & residual8 elements
Fe Iron≤ 2%
Cr Chromium≤ 1%
C Carbon≤ 0.02%
Si Silicon≤ 0.1%
Co Cobalt≤ 1%
Mn Manganese≤ 1%
P Phosphorus≤ 0.04%
S Sulphur≤ 0.03%

Mechanical minima by form

Guaranteed values differ by form, size and delivery condition; quotations confirm the specification, form, size and condition.

FormCondition Rm MPaRp0.2 MPaA ≥ %Other requirements and notes
Bar and forgings
BarAnnealed and descaled ≥ 760 (110 ksi) ≥ 350 (51 ksi) ≥ 40
Plate, sheet and strip
Plate, sheet and stripSolution annealed ≥ 760 (110 ksi) ≥ 350 (51 ksi) ≥ 40
Tube and pipe
Seamless pipe and tubeSolution annealed and descaled ≥ 760 (110 ksi) ≥ 350 (51 ksi) ≥ 40
Welded pipe and tubeSolution annealed ≥ 760 (110 ksi) ≥ 350 (51 ksi) ≥ 40
Fittings and flanges
Fittings (factory-made wrought butt-weld / socket)1950 °F [1065 °C] minimum, rapid air or water quench — — — Tensile properties follow the starting material.
No tension test on the finished fitting unless agreed.
Minimum temperature.

Hardness requirement

Informative only — not a basis for acceptance — ≤ 100 HRB (sheet, strip and plate, annealed)

⚠ This is not an acceptance criterion.

More detail 2

Hardness values are for information only and are not a basis for rejection or acceptance.

The binding requirements in that table are the tensile ones: for Hastelloy B-2, both sheet and strip (under 4.76 mm) and plate (4.76–63.5 mm) require ≥760 MPa tensile, ≥350 MPa yield and ≥40% elongation.

Grain size

Required by the standard, conditionally — Annealed sheet and strip: mean grain diameter ≤0.127 mm at t ≤3.175 mm; ≤0.214 mm above 3.175 mm

Applies to annealed sheet and strip only; plate and the other product forms are not assessed.

More detail 2

The mean-grain-diameter column is a maximum in both standards and carries identical values, so it is unambiguous; this entry is therefore stated in terms of diameter.

The contradiction in the grain-size-number column is a printing matter: an order that is to be accepted on the number must state in the contract which standard and which column governs.

Where this grade is recommended

Matched in 3 service conditions; ranks and scores computed from the condition-scoring matrix.

Service conditionIndustry TemperatureRankScore
HCl & reducing acids Chemical Processing ≤ 60 °C 1 / 8 95
Acidizing & fracturing (HCl/HF) Oil & Gas ≤ 120 °C 1 / 6 94
Hydrofluoric acid Chemical Processing ≤ 50 °C 6 / 6 78

Designations & equivalents

W.Nr. (Germany)2.4617
EN designationNiMo28
Trade name(s)Hastelloy B-2 / Nimofer 6928
ASTM / AISIB333 / B335 / B366 / B462 / B564 / B619 / B622

Cross-references are common near-equivalents for search and shortlisting; substitution across standards requires clause-by-clause verification. All grades in one cross-reference table →

Applicable standards

7 specifications. Name the standard and its edition on the order.

Guaranteed values and required tests differ between specifications — see Mechanical minima by form for the figures per form.

Frequently asked questions

What is Alloy B-2 · UNS N10665?

Alloy B-2 · UNS N10665 — Ni corrosion-resistant. Ni-Mo type — dedicated to hydrochloric and reducing acids

What is the maximum service temperature of N10665?

Typically about 540 °C; the practical limit depends on media, stress and design life — acceptance per the governing standard.

What is the tensile strength of N10665?

The specified minimum tensile strength is 760 MPa for the main product form. Minima for other forms and sizes are listed under "Mechanical minima by form" on this page.

Which standards cover N10665?

ASTM B333, ASTM B335, ASTM B366, ASTM B462, ASTM B564 (forgings), ASTM B619, ASTM B622

Where is N10665 typically used?

HCl & reducing acids (Chemical Processing); Acidizing & fracturing (HCl/HF) (Oil & Gas); Hydrofluoric acid (Chemical Processing)

In which forms is N10665 available?

Tube, plate, strip, bar, forgings, wire and other forms — sizes and delivery condition confirmed per order, with EN 10204 3.1 / 3.2 certification.

Same series

Download PDF datasheet

This grade’s datasheet as an A4 PDF — for filing, printing or forwarding to colleagues.

Download PDF datasheet

Supply & enquiry

Tube & pipeφ1 – 219 × 0.25 – 25 mmPlate4.76 – 80 mmBarφ8 – 300 mmWire & filler metalsφ0.01 – 8 mm

For this grade we can supply, against your service conditions:

Or email us: info@kochlin.com