X1NiCrMoCu31-27-4 · UNS N080281.4563 · Alloy 28

Dual-duty grade — sour-well tubing and wet-process phosphoric acid

Super-austenitic stainless
Units
Tensile Rm
500
MPa · ≥ std. min
Yield Rp0.2
214
MPa · ≥ std. min
Elongation A
40
% · ≥ std. min
Service limit
400
°C · indicative max
Density
8
g/cm³

Physical properties

Density8.0g/cm³
Modulus E195 / 190 / 182 / 174 / 166 / 158GPa @ 20 / 100 / 200 / 300 / 400 / 500 °C
Thermal conductivity12W/(m·K) @ 20 °C
Thermal expansion15.8 / 16.1 / 16.5 / 16.9 / 17.310⁻⁶/K, mean 20-100 / 20-200 / 20-300 / 20-400 / 20-500 °C
Specific heat450J/(kg·K) @ 20 °C
Resistivity1.00Ω·mm²/m @ 20 °C

Informative values: they vary with composition, condition and test method. Use the governing standard or measured mill data for pressure and heat-transfer calculations.

Values are taken from EN 1.4563 (the same alloy) and are informative.

14016018020020100200300400500GPaTemperature °CModulus E14016018020020100200300400500GPaTemperature °CModulus E14016018020020100200300400500GPaTemperature °CModulus E
15.516.016.517.017.510020030040050010⁻⁶/KTemperature °CMean expansion α15.516.016.517.017.510020030040050010⁻⁶/KTemperature °CMean expansion α15.516.016.517.017.510020030040050010⁻⁶/KTemperature °CMean expansion α
Each point is the mean from 20 °C to that temperature.

Chemical composition

Fe 33%Ni 32%Cr 27%Mo 3.5%Cu 1%Minor & residual 3.6%

Nominal: mid-range where both limits are given, the cap where only a maximum is, balance takes the remainder. Exact specified ranges below.

ElementName Content %
Main elements5 elements
Fe IronBal.
Ni Nickel30 – 34%
Cr Chromium26 – 28%
Mo Molybdenum3 – 4%
Cu Copper0.6 – 1.4%
ElementName Content %
Minor & residual5 elements
C Carbon≤ 0.03%
Si Silicon≤ 1%
Mn Manganese≤ 2.5%
P Phosphorus≤ 0.03%
S Sulphur≤ 0.03%

Mechanical minima by form

Guaranteed values differ by form, size and delivery condition; quotations confirm the specification, form, size and condition.

FormCondition Rm MPaRp0.2 MPaA ≥ %Other requirements and notes
Bar and forgings
Bars (EN 10088-3, ≤160 mm)+AT (solution annealed) 500 – 750 ≥ 220 ≥ 35 Also specified: Hardness ≤ 230 HBW
Rp1.0 ≥ 250 MPa; KV ≥ 100 J longitudinal; 160–250 mm: transverse A ≥ 30 %, KV ≥ 60 J.
Plate, sheet and strip
Plate, sheet and stripSolution annealed and rapidly cooled ≥ 500 (73 ksi) ≥ 214 (31 ksi) ≥ 40
Plate, sheet and strip for pressure vessels and general useAnnealed ≥ 500 (73 ksi) ≥ 214 (31 ksi) ≥ 40 Also specified: Hardness ≤ 90 HRB
Hot-rolled plate (EN 10088-2, ≤75 mm)+AT (solution annealed) 500 – 700 ≥ 220 ≥ 40 Rp1.0 ≥ 260 MPa; hot-rolled plate only. KV ≥ 100/60 J (long./transv., over 10 mm).
Tube and pipe
Seamless pipe and tubeRecommended: solution treated at 1080–1150 °C, water quenched or rapidly cooled ≥ 500 (73 ksi) ≥ 214 (31 ksi) ≥ 40
Seamless and welded pressure tubes (EN 10216-5 / EN 10217-7, wall ≤60 mm)+AT (solution annealed) 500 – 750 ≥ 215 ≥ 40 Rp1.0 ≥ 245 MPa; transverse A ≥ 35 %; KV ≥ 120/90 J (long./transv.).

Where this grade is recommended

Matched in 2 service conditions; ranks and scores computed from the condition-scoring matrix.

Service conditionIndustry TemperatureRankScore
Downhole tubing (sour H₂S/CO₂) Oil & Gas > 230 °C 3 / 10 89
Phosphoric acid Chemical Processing 80 – 200 °C 2 / 7 88

Designations & equivalents

W.Nr. (Germany)1.4563
EN designationX1NiCrMoCu31-27-4
Trade name(s)Alloy 28 / Sanicro 28
ASTM / AISIA240 / B668 / B709

Cross-references are common near-equivalents for search and shortlisting; substitution across standards requires clause-by-clause verification. All grades in one cross-reference table →

Applicable standards

7 specifications. Name the standard and its edition on the order.

Guaranteed values and required tests differ between specifications — see Mechanical minima by form for the figures per form.

Frequently asked questions

What is Alloy 28 (Sanicro 28) · UNS N08028?

Alloy 28 (Sanicro 28) · UNS N08028 — Super-austenitic stainless. Dual-duty grade — sour-well tubing and wet-process phosphoric acid

What is the maximum service temperature of N08028?

Typically about 400 °C; the practical limit depends on media, stress and design life — acceptance per the governing standard.

What is the tensile strength of N08028?

The specified minimum tensile strength is 500 MPa for the main product form. Minima for other forms and sizes are listed under "Mechanical minima by form" on this page.

Which standards cover N08028?

ASTM B709, ASTM B668, ASTM A240/A240M, EN 10088-2 (sheet, plate, strip), EN 10088-3 (bar, rod, wire, sections), EN 10216-5 (seamless pressure tubes), EN 10217-7 (welded pressure tubes)

Where is N08028 typically used?

Downhole tubing (sour H₂S/CO₂) (Oil & Gas); Phosphoric acid (Chemical Processing)

In which forms is N08028 available?

Tube, plate, strip, bar, forgings, wire and other forms — sizes and delivery condition confirmed per order, with EN 10204 3.1 / 3.2 certification.

Same series

Download PDF datasheet

This grade’s datasheet as an A4 PDF — for filing, printing or forwarding to colleagues.

Download PDF datasheet

Supply & enquiry

Tube & pipeφ1 – 219 × 0.25 – 25 mmPlate4.76 – 80 mmBarφ8 – 300 mmWire & filler metalsφ0.01 – 8 mm